W-Ti-C-N계 초경 복합재의 제조와 내마모성 및 기계적 성질 |
박상희, Helmut Holleck1 |
부산대학교 무기재료공학과 1Karlsruhe 핵연구센타 재료 및 고체재료연구소 |
Preparation, Wear Resistance and Mechanical Properties of W-Ti-C-N Based Hard Materials |
|
|
|
|
|
ABSTRACT |
W-Ti-C-N based multiphase hard materials have been prepared from WC/TiN powder mixture. By sintering at and above 190$0^{circ}C$, the two phases of powder mixture has transformed into intermixed W, W2C and Ti(C, N) phases. For the temperature range between 180$0^{circ}C$ and 210$0^{circ}C$, the sintered or hot pressed samples show maximum density and hardness. The seems that metallic W grains enhance the fracture toughness of materials. The wear resistance of the material is found to increase with increasing hardness. |
|